摘要
研究了不同Al-Si镀层去除状态下Usibor 1500钢激光拼焊后和热成形后焊接接头的组织特征, 并采用室温拉伸试验测试了热成形后焊接接头的力学性能。结果表明, 拼焊后的焊缝区显微组织为粗大板条马氏体和在光学显微镜下呈白色不均匀的第二相,白色相随着去除镀层部位的增多而减少。接头拉伸断裂模式与焊缝中白色相的分布情况相关。镀层去除状态对激光拼焊板性能有着显著影响, 上表面镀层的去除可显著提升接头性能; 随着下表面镀层去除部位的增多, 接头拉伸性能提升, 且在上下表面镀层全部去除的情况下, 接头的抗拉强度达到最大。
Abstract
The microstructure features of welded joints after laser tailor-welding and hot stamping of Usibor 1500 steels are investigated. The mechanical properties of welded joints after hot stamping are tested by the room temperature tensile test. The results show that the microstructure of the weld seam is composed of coarse lath martensite and the unevenly distributed second phase with white color under the optical microscope. The white phase number decreases with the increase of coating removal parts. The tensile fracture pattern of the welded joint is related to the distribution of white phase in the weld seam. The removal state of coating has a significant effect on the performance of laser tailor-welded blanks. The removal of upper coating can significantly improve the performance of welded joints. The tensile property of welded joints is significantly improved with the number of the lower coating removal parts increases. The tensile strength of welded joint reaches the maximum value when all of the coatings are removed.
参考文献

[1] Karbasian H, Tekkaya A E. A review on hot stamping[J]. Journal of Materials Processing Technology, 2010, 210(15): 2103-2118.

[2] Merklein M, Lechler J, Geiger M. Characterisation of the flow properties of the quenchenable ultra high strength steel 22MnB5[J]. CIRP Annals-Manufacturing Technology, 2006, 55(1): 229-232.

[3] Kang M, Kim C, Bae S M. Laser tailor-welded blanks for hot-press-forming steel with arc pretreatment[J]. International Journal of Automotive Technology, 2015, 16(2): 279-283.

[4] 刘国承, 田杰平, 史玉升, 等. 汽车用钢焊接技术研究进展[J]. 激光与光电子学进展, 2015, 52(1): 010004.

    Liu Guocheng, Tian Jieping, Shi Yusheng, et al. Review of welding technologies for automotive steel sheets[J]. Laser & Optoelectronics Progress, 2015, 52(1): 010004.

[5] 魏 菁, 王 欢, 石少坚, 等. 10CrSiNiCu船用高强钢光纤激光焊接接头组织和性能[J]. 中国激光, 2016, 43(3): 0303003.

    Wei Jing, Wang Huan, Shi Shaojian, et al. Microstructure and properties of fiber laser wire welded joints of 10CrSiNiCu high strength shipbuilding steel[J]. Chinese J Lasers, 2016, 43(3): 0303003.

[6] Jia J, Yang S L, Ni W Y, et al. Microstructure and mechanical properties of fiber laser welded joints of ultrahigh-strength steel 22MnB5 and dual-phase steels[J]. Journal of Materials Research, 2014, 29(21): 2565-2575.

[7] 伍 强, 徐兰英, 杨永强, 等. 高强钢激光焊接残余应力的研究[J]. 中国激光, 2015, 42(6): 0603007.

    Wu Qiang, Xu Lanying, Yang Yongqiang, et al. Study on laser welding residual stress of high strength steel[J]. Chinese J Lasers, 2015, 42(6): 0603007.

[8] Kim C H, Choi J K, Kang M J, et al. A study on the CO2 laser welding characteristics of high strength steel up to 1500 MPa for automotive application[J]. Journal of Achievements in Materials and Manufacturing Engineering, 2010, 39(1): 79-86.

[9] 张 帆, 李 芳, 华学明, 等. Al-Si镀层在激光拼焊板焊缝中分布及性能影响研究[J]. 中国激光, 2015, 42(5): 0503005.

    Zhang Fan, Li Fang, Hua Xueming, et al. Research of effects with Al-Si coating on distribution and performance of tailored laser[J]. Chinese J Lasers, 2015, 42(5): 0503005.

[10] Iordachescu D, Blasco M, Lopez R, et al. Recent achievements and trends in laser welding of thin plates[J]. Journal of Optoelectronics and Advanced Materials, 2011, 13(7-8): 981-985.

[11] Kim C, Kang M J, Park Y D. Laser welding of Al-Si coated hot stamping steel[J]. Procedia Engineering, 2011,10: 2226-2231.

[12] Lee M S, Moon J H, Kang C G. Investigation of formability and surface micro-crack in hot deep drawing by using laser-welded blank of Al-Si and Zn-coated boron steel[J]. Proceedings of the Institution of Mechanical Engineers Part B, 2014, 228(4): 540-552.

[13] Norman P, Wiklund G, Janiak P, et al. Comparison of 22MnB5-steel with and without AlSi-coating during laser hybrid arc welding[C]. Conference on Laser Materials Processing in the Nordic Countries, 2011, 13.

[14] Kang M, Kim C, Lee J. Weld strength of laser-welded hot-press-forming steel[J]. Journal of Laser Applications, 2012, 24(2): 022004.

[15] Davis C L, King J E. Cleavage initiation in the intercritically reheated coarse-grained heat-affected zone: Part I. Fractographic evidence[J]. Metallurgical and Materials Transactions A, 1994, 25(3): 563-573.

[16] Kang M, Kim Y M, Kim C. Effect of heating parameters on laser welded tailored blanks of hot press forming steel[J]. Journal of Materials Processing Technology, 2016, 228: 137-144.

陈晓莞, 李芳, 林文虎, 金鑫, 华学明. 硼钢镀层对热成形激光拼焊板组织及性能的影响[J]. 中国激光, 2017, 44(4): 0402011. Chen Xiaoguan, Li Fang, Lin Wenhu, Jin Xin, Hua Xueming. Effect of Boron Steel Coating on Microstructure and Property of Laser Tailor-Welded Blanks After Hot Stamping[J]. Chinese Journal of Lasers, 2017, 44(4): 0402011.

关于本站 Cookie 的使用提示

中国光学期刊网使用基于 cookie 的技术来更好地为您提供各项服务,点击此处了解我们的隐私策略。 如您需继续使用本网站,请您授权我们使用本地 cookie 来保存部分信息。
全站搜索
您最值得信赖的光电行业旗舰网络服务平台!